Thursday, April 12, 2012

Degumming/Scouring Process of Silk

sheen, color, hand, and texture of the silk. Because the gum can serve as a protective layer, it is typically left on the silk until it is ready to dye. In some cases, the fabric is woven to completion, and then degummed, to protect the yarn from abrasion on the loom. The process involved to remove these impurities is called ‘degumming’ or ‘scouring’ of silk. 

 











Silk

The composition of raw silk is as follows: 

Fibroin - 70-80% 
Sericin - 20-305 
Waxy matter - 0.4-0.8% 
Carbohydrates - 1.2-1.65 
Inorganic matter - 0.7% 
Pigment - 0.2% 


The process of eliminating “Gum (sericin)” from raw silk is known as degumming of silk. Degumming of silk involves mainly the removal of sericin from the fibroin. Sericin is insoluble in water. It is comparatively easily hydrolyzed, whereby the long protein molecule of sericin, is broken down into smaller fractions, which are easily dispersed or solubillsed in hot water. 


Typical Recipe for Silk Degumming: 


Wetting agent……………………=0.5-1.0 g/l 
Sequestering agent…………….=1.0-2.0 g/l 
Antifoaming agent……………...=0.5-1.0 g/l 
Natural soap…………………….=15.0-30.0 g/l 
TSP/Soda ash…………………..=1.0-3.0 g/l 
Detergent………………………..=1.0-3.0 g/l (not mandatory if use soda) 
Temperature…………………….=90-95°C 
Time………………………………=90-120 min 
pH…………………………………=9.5-10.5 
M:L………………………………..=1:10 


Working Procedure:



  1. Set the bath with substrate at room temperature and add soap and other necessary auxiliaries.

  2. If necessary add trisodium phosphate (TSP) or soda ash to maintain desired pH 9-10.

  3. Raise the temperature to 95° and run for 2 hours for optimum removal of sericin gum.

  4. Cool down to 70°C and then drop the bath.

  5. Wash it with warm and cold water successively. 

5 Textile Technology: Degumming/Scouring Process of Silk sheen, color, hand, and texture of the silk. Because the gum can serve as a protective layer, it is typically left on the silk until it is r...
Tags:

No Comments

***www.TextileTune.blogspot.Com***

< >
Accessories (10) acrylic (1) After treatment (2) Apparel Manufacturing (1) azoic dye (1) basic dye (2) beating (1) blend dyeing (2) Blowroom (5) calculation (2) Cam (1) Campus news (5) carbon fiber (1) Carding (6) Class Lecture (1) color (5) Combing (2) cotton (3) count (3) crimp (1) defects (6) Denim Process (2) Dictionary (26) direct dye (2) disperse dye (11) dye (1) dyeing (15) dyeing auxiliaries (8) dyeing m/c (9) Ebooks (6) Experiment (3) Fabric (4) Fabric Manufacturing (12) Fabric structure (11) Factory (9) fastness (7) Fastness test (7) finishing m/c (4) FlowChart (3) foam dyeing (1) FSD (12) garment dyeing (2) Garments (3) Garments m/c (10) glass fiber (2) hemp (1) inspection (3) Interlinning (1) Interview Q (6) jute (9) jute spinning (13) knit dyeing (1) knitting m/c (21) lecture sheet (1) loom (9) Man made fiber (1) Marchandising (5) milk fiber (1) Modern Textiles (1) mordant dye (1) naphthol dye (1) Needle (2) Others (1) Pattern (2) picking (2) pigment (5) pre-treatment (11) printing amp; finishing (8) printing m/c (1) properties (6) rayon (2) reactive dye (11) Recent News (17) RingFrame (9) Sample (1) seam (1) sewing (3) shedding (3) silk (1) Simplex (6) Sinker (3) sizing (10) Spinning m/c (13) stitch (4) stop motion (4) sulpher dye (9) Technical textile (13) Testing m/c (13) textile definition (7) Textile Industry (1) Textile Physics (2) textiletechnology (18) thread (1) tie dye (1) trimming (1) TTQC (21) twill (4) twist (3) Uster m/c (1) vat dye (4) warp knitting (7) warping (8) washing (2) wastage (2) water (2) Weaving (16) weft knitting (2) Wet Process (1) Winding (11) wool (2) Yarn (30)